CHEMICAL COMPOSITION
Grades according to
EN 10025-5 |
Heat analysis in % | |||||||||
---|---|---|---|---|---|---|---|---|---|---|
CMAX | Mn | Si | P | SMAX | AlMIN | Cr | Cu | NMAX | CEVMAX | |
S355J0WP | 0,12 | 1,0 | 0,75 | 0,06 - 0,15 | 0,035 | - | 0,30 - 1,52 | 0,25 - 0,55 | 0,012 | 0,52 |
S355J2WP | 0,030 | 0,020 | - | 0,52 |
Grades according to
TN USSK 10025-5 |
Heat analysis in % | ||||||||
---|---|---|---|---|---|---|---|---|---|
CMAX | Mn | Si | P | SMAX | AlMIN | Cr | Cu | NiMAX | |
KONOX 345HR | 0,12 | 0,20 - 0,55 | 0,25 - 0,55 | 0,07 - 0,15 | 0,015 | 0,02 | 0,50 - 1,20 | 0,25 - 0,60 | 0,65 |
MECHANICAL PROPERTIES
Grades according to EN 10025-5 |
ReH [MPa] |
Rm [MPa] | AMIN (%) | KVMIN [J] | ||||
---|---|---|---|---|---|---|---|---|
a < 3 | a ≥ 3 | L0 = 80 mm | L0 = 5,65√S0 | |||||
a ≤ 2 | 2 < a ≤ 2,5 | 2,5 < a < 3 | a ≥ 3 | |||||
S355J0WP | 355 | 510 - 680 | 490 - 630 |
l 16 t 14 |
l 17 t 15 |
l 18 t 16 |
l 22 t 20 |
0˚C 27 |
S355J2WP | -20˚C 27 |
Grades according to TN USSK 10025-5 |
RP0,2 [MPa] |
Rm [MPa] | AMIN (%) | Bend test | ||
---|---|---|---|---|---|---|
L0 = 80 mm | L0 = 5,65√S0 | α | D | |||
KONOX 345HR | 345 | 485 | 20 | 22 | 180° | 1a |
- THICKNESS TOLERANCES IN ACCORDANCE WITH EN 10051 AND U. S. STEEL KOŠICE, S.R.O.
- SHEET FLATNESS TOLERANCES IN ACCORDANCE WITH EN 10051